[MW:6298] MW: - 6265-Re: Application of B-31G-Strength of corroded Pipe


Dear  Rahul,

 

In your case ASME B31G would not be the right code. B 31G is an excellent code primarily developed for fitness for service evaluation of above and underground hydrocarbon pipelines(liquid or gas). The fitness margins in these codes will not necessarily be the same for above ground process piping where failures  could be catastrophic.

 

A combination of API-570 and API/ASME -579 would enforce  better  integrity and remaining life of corroded process plant piping. If it is one to time fitness for service evaluation for corroded pipes API-579 is the ideal code. One can perform Level-1, Level-2 and  Level-3 design calculations and validate the remaining life of any component, e.g. pressure vessels and pressure piping. Level-1 & Level-2 is formula based calculations, with different levels of safety margins, Level-3 is calculation plus the FEA analysis.

 

For  long term corrosion and Plant life , corrosion inspection programme as per API-570 would be recommended.

 

API-579 was originally developed for oil and gas industries. ASME adopted this code in 2007, as post construction code. I attended  few trainings with API in 2006/2007, and use this code for component integrity purpose whenever the need arises.

 

I have attached some extracts from ASME B-31G and API/ASME-579  and API-570 for your reference.

 

Feel free to raise any question.

 

 

Thanks

 

Pradip Goswami, P.Eng.

Welding & Metallurgical Engineer/Specialist

Ontario Power Generation Inc.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 

 

 

-----Original Message-----

From: materials-welding@googlegroups.com

[mailto:materials-welding@googlegroups.com] On Behalf Of hpi001

Sent: Monday, August 02, 2010 3:51 PM

To: Materials & Welding

Subject: [MW:6265] Re: Application of B31G - Strength of corroded Pipe

 

Dear Rahul,

 

In my opinion you are correct, the minimum allowed wall thickness is the nominal wall thickness including manufacturing tolerances, minus the corrosion allowance which is taken into account during design calculation.

I'm not that familiar with ASME but when pressure vessels and / or piping are designed under the European Pressure Equipment Directive the minimum thickness never is allowed to be less than the value taken into account during calculations.

However if ASME B31G is applicable to the existing piping and you can guarantee proper and safe operation by way of calculations given in this ASME part and based on the wall thickness found during actual measurements than I would say way not using that possibility to extend the piping's lifetime.

 

Best Regards,

 

Herman Pieper

 

On 2 aug, 14:05, "Pisat, R. (Rahul)" <Rahul.Pi...@akzonobel.com>

wrote:

Dear all,

 

One of plant project engineer has asked me to make document for Minimum required wall thickness for the piping  which is acceptable to run the process with defined design condition under corroded condition.

 

As per my understanding this the same Min. wall thickness based on calculation of required wall thickness for design pressure and design temperature .i.e. Min. wall thickness which is ( Nominal wall thickness - manufacturing tol..- Corrosion allowance ).

 

But one of our old engineering manual has listed the use of ASME B31G manual for determining the remaining strength of corroded Pipelines,  after reading this manual , I can state that this manual gives the strength of corroded portion of the pipeline. Defined parameters in this specification is based on Depth of corrosion and length of the metal loss.

 

My query is how can I use this ASME B31G for defining the minimum required wall thickness requirement for existing piping network in plant.

 

Do you agree that my initial assumption of Min. wall thickness i.e.  Nominal wall thickness - Mfr. Toll. - Corrosion allowance is a right approach ?

 

Waiting for your suggestions.

 

reg

 

Rahul

 

--

To post to this group, send email to materials-welding@googlegroups.com

To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/

The views expressed/exchanged in this group are members personal views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


THIS MESSAGE IS ONLY INTENDED FOR THE USE OF THE INTENDED RECIPIENT(S) AND MAY CONTAIN INFORMATION THAT IS PRIVILEGED, PROPRIETARY AND/OR CONFIDENTIAL. If you are not the intended recipient, you are hereby notified that any review, retransmission, dissemination, distribution, copying, conversion to hard copy or other use of this communication is strictly prohibited. If you are not the intended recipient and have received this message in error, please notify me by return e-mail and delete this message from your system. Ontario Power Generation Inc.

No comments:

Re: [MW:34913] Filler wire

E71T-1C  is Charpy Impact tested at -20degC E71T-1CJ is Charpy impact tested at -40degC. AWS Classification for FCAW is only a supplementary...