Section IX.
"More than one WPS having different essential, supplementary
essential, or nonessential variables may be used in a single
production joint. Each WPS may include one or a combination of
processes, filler metals, or other variables (QW200.4)" => This is
exactly under the heading of "Combination of Procedures" in ASME
Section IX. Hence both the terminalogies are correct.
Straight reply to your Manoj's query is "Yes, it is possible" provided
the thickness limit shall satisfy your new procedure; as Bathula
rightly said, you can make a new WPS with existing two PQR's as
supporting PQRs.
Thanks
Senthil
On Aug 10, 8:43 am, "Bathula Raghuram (Mumbai - PIPING)"
<R.Bath...@ticb.com> wrote:
> First it is not a question of combining WPS's. You can write multiple WPS using multiple PQR's. in this case either you can use the same or prepare a separate WPS with the said combination, as long as all other essential variables (such as T and t limits) as per supporting PQR's.
>
> More than one WPS having different essential, supplementary essential, or nonessential variables may be used in a single production joint. Each WPS may include one or a combination of processes, filler metals, or other variables (QW200.4)
> ________________________________
> From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of manoj john
> Sent: Tuesday, August 10, 2010 8:50 AM
> To: materials-welding@googlegroups.com
> Subject: [MW:6404] COMBINED WPS & pqr
>
> Dear All,
>
> I have the following qualified WPS as per ASME sec. IX
>
> 1) Material Group : P1 (pipe - without backgouging)
> Welding process : SMAW
> Filler Metal : E 6010 Root run and E 7018 Subsequent run
>
> 2) Material group : P1 (plate - with back gouging)
> Welding process : FCAW
> Filler Metal : E71T
>
> Can I combine these above two WPS to weld Pipe of material SA 106 Gr B root run with SMAW E6010 and subsequent run FCAW E71T .
>
> Thank you with warm Regards,
> Manoj
>
> Filtered by Hosted Filtering
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
No comments:
Post a Comment