Please find the way of welding dissimilar metals article.
Prasanna
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Ashfaq Anwer
Sent: 12 August 2010 16:30
To: materials-welding@googlegroups.com
Subject: Re: [MW:6467] P42 (Monel) to P1 (SA516 G.70) Welding
What is the type of joint? Shell to nozzle with groove and fillet reinforcement? Nozzle thickness?
Normally, welding of P42 and P1 is made without any PWHT operation.
Just perform the weld with the wires / electrodes you mentioned and get the procedure qualified. No need to butter the P1 side otherwise, you may need to consider PWHT after buttering.
Regards,
Ashfaq
thepetrostreet.com
On Thu, 12 Aug 2010 12:13:31 +0400, Muhammed Ibrahim PK <ibratech@gmail.com> wrote:
Gents,
We have to weld a monel Nozzle SB165 (UNS N04400) (P No.42) to SA516G.70 (PNo.1) 45 mm thk
The vessel is required PWHT.
I need to qualify a PQR for this welding with ERNiCu+ENiCu-7.
Is it required to do PWHT of this joint (P42 to P1)?.
If PWHT is required what is the way of welding of this joint?
If PWHT is not required what is the procedure to weld it?
Is it required to butter the CS with monel before butt welding?
Is any post heting is required for this joint?
Thanks & Regards
Muhammed Ibrahim PK
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
__________ Information from ESET NOD32 Antivirus, version of virus signature database 5359 (20100811) __________
The message was checked by ESET NOD32 Antivirus.
http://www.eset.com
__________ Information from ESET NOD32 Antivirus, version of virus signature database 5365 (20100813) __________
The message was checked by ESET NOD32 Antivirus.
http://www.eset.com
__________ Information from ESET NOD32 Antivirus, version of virus signature database 5365 (20100813) __________
The message was checked by ESET NOD32 Antivirus.
http://www.eset.com
No comments:
Post a Comment