Hi,

Backing strips are expensive and sometimes fall of or pushed of if the wire goes through the gap.

If you have to Xray and I am sure you do if building to API650 then it is better to back grind and back weld.

Miller have a metal cored wire that runs under a sub arc flux and can take a gap we are testing it on our tanks for HORZ. Welds.

It is difficult to punch even 6mm in the horz because of the speed you have to travel at to avoid cold lapping, so we have found it best to back grind and weld.

BR

Lusky

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of vipin george
Sent: Sunday, August 08, 2010 6:35 PM
To: materials-welding@googlegroups.com
Subject: **** SPAM **** Re: [MW:6378] SAW WELDING

 

Hi!
Yes ! you can , but use backing strips .

Rgds
VG

On Sun, Aug 8, 2010 at 6:54 PM, Eng/ Mostafa Kamel Hussein <mkh_200@yahoo.com> wrote:

Can i make single pass full penetration with SAW without GMAW back weld in circumferential welds in tank with 6mm in thickness and the groove is square with 1mm gab??? 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


This e-mail and any files transmitted with it are confidential and intended solely for the use of the individual or entity to whom they are addressed. If you have received this e-mail in error please notify the system manager. Please note that any views or opinions presented in this e-mail are solely those of the author and do not necessarily represent those of the company. Finally, the recipient should check this e-mail and any attachments for the presence of viruses. The company accepts no liability for any damage caused by any virus transmitted by this e-mail.



This e-mail and any files transmitted with it are confidential and intended solely for the use of the individual or entity to whom they are addressed. If you have received this e-mail in error please notify the system manager. Please note that any views or opinions presented in this e-mail are solely those of the author and do not necessarily represent those of the company. Finally, the recipient should check this e-mail and any attachments for the presence of viruses. The company accepts no liability for any damage caused by any virus transmitted by this e-mail.

No comments:

[MW:34866] Presentation for WPS ,PQR AND WPQ as per ASME Sec IX in power point

Dear Experts.        If anyone having presentation of WPS,PQR and WPQ  as per ASME  SEC.IX  in power point then please share . Regards Sanja...