RE: [MW:9084] Re: Repair of Body cracks for A 217 Gr WC6

Vinod,

I would say that was a wise discussion. Although I had dropped a few lines on safe welding practices as per API -510, later after browsing through API-579(Section-11, Assessment of Fire Damage ), I realized that a lot more things are desired for proper assessment for any fire damage , then only any welding/ refurbishing should be thought of.

It would be a good idea to get some heads up from API-579 on such damages in future . There're are some typical  examples on assessment of fire damages of various plants and equipments in this API/ASME book.

Thanks.


Pradip Goswami,P.Eng.,IWE
Welding & Metallurgical Specialist & Consultant
Email-pgoswami@sympatico.ca,
pgoswami@quickclic.net

-----Original Message-----
From: materials-welding@googlegroups.com [
mailto:materials-welding@googlegroups.com] On Behalf Of Vinod Jotwani
Sent: Tuesday, January 04, 2011 7:14 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:9083] Re: Repair of Body cracks for A 217 Gr WC6

Dear All,

Thanks for the valuable suggestions. Looking to the risk involved and the time period required to carry out the repair we have decided to put in a globe valve to control flow temperorily (as process allows for it) and to procure new valve body.

Thanks again,

Vinod

--- On Mon, 1/3/11, Marcelo P. Soriano Qa/Qc Eng'r. <marcelopsoriano_1925@yahoo.com.ph> wrote:

> From: Marcelo P. Soriano Qa/Qc Eng'r.
> <marcelopsoriano_1925@yahoo.com.ph>
> Subject: [MW:9064] Re: Repair of Body cracks for A 217 Gr WC6
> To: "Materials & Welding" <materials-welding@googlegroups.com>
> Date: Monday, January 3, 2011, 4:25 PM Please be practical (MULTIPLE
> CRACKS)????
>
> 1. need pqr, wps and qualified welder.
> 2. 2500 rating
> 3. time for the preparation of documents to be use for repair 4.
> testing
>
> OR
>
> 1. Purchase valve and reinstall and back to operation as early than to
> repair MULTIPLE CRACKS on VALVE BODY....
>
>
>
> On Jan 3, 12:56 pm, Muni Andy <cmkf...@gmail.com>
> wrote:
> > Dear Marcelo Soriano,
> > ASTM A217 permits repair welding.
> > We can do repair with approved welding Procedure and
> qualified welder.
> > Regards,
> > C.Muniyandi
> > Surveyor
> > Coimbatore
> >
> > On Mon, Jan 3, 2011 at 1:50 PM, Marcelo P. Soriano
> Qa/Qc Eng'r. <
> >
> >
> >
> > marcelopsoriano_1...@yahoo.com.ph>
> wrote:
> > > dear members,
> >
> > > in my opinion and experience theres bo any code
> telling that repairing
> > > welding of valve body* (casting) because in
> casting if you have crack
> > > on it and apply heat it will be larger and more
> cracks will run
> > > through the body, its better to replace it that
> than compromise the
> > > safety and property.....
> >
> > > thanks,
> > > marcelo soriano
> > > Technip Qc Eng'r
> >
> > > On Jan 2, 7:27 am, Vinod Jotwani <pooj...@yahoo.com>
> wrote:
> > > > Dear All,
> >
> > > > We have noticed multiple crack during the
> replica check in the control
> > > valve body ( Material A 217 Gr WC6 , size 2 " X
> 2500 RTJ, H2 service) during
> > > the fire incident at our Hydrocracker plant.  We
> would like to carry out the
> > > repair jobs for the same,
> >
> > > > Kindly share your experience and also advise
> whether advisable or not.
> > > Also share the WPS and cautions to be followed if
> repair performed by anyone
> > > in the group.
> >
> > > > Vinod
> >
> > > --
> > > To post to this group, send email to
> > > materials-welding@googlegroups.com
> > > To unsubscribe from this group, send email to
> > > materials-welding+unsubscribe@googlegroups.com<materials-welding%2
> > > materials-welding+Bunsubscr­ibe@googlegroups.com>
> > > For more options, visit this group's bolg at
> > >
http://materials-welding.blogspot.com/
> > > The views expressed/exchnaged in this group are
> members personel views and
> > > meant for educational purposes only, Users must
> take their own decisions
> > > w.r.t. applicable code/standard/contract
> documents.- Hide quoted text -
> >
> > - Show quoted text -
>
> --
> To post to this group, send email to
> materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
>
http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views
> and meant for educational purposes only, Users must take their own
> decisions w.r.t. applicable code/standard/contract documents.
>


     

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34866] Presentation for WPS ,PQR AND WPQ as per ASME Sec IX in power point

Dear Experts.        If anyone having presentation of WPS,PQR and WPQ  as per ASME  SEC.IX  in power point then please share . Regards Sanja...