Re: [MW:9201] RE: 9171] API 530 Solution annealing after coiling of SA213 TP304H

Mr.Goswami,
Thanks for your reply.
Design code-API530. Const.Code - ASME Sec.VIII,Div.1/B31.3
Acc.to Con.Code,I have gone thru UHA44 and B31.3 regarding this case,i found B31.3 doesnt require any post heatreatment in this case as well as UHA44 of Sec.VIII,Div1 calculated Strain percentage is less than 10%.So doesnt need to do Post heat treatment.
 
Actually API530 is a design code
 
Thanks for your inputs.

Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Thu, 1/13/11, pgoswami <pgoswami@quickclic.net> wrote:

From: pgoswami <pgoswami@quickclic.net>
Subject: [MW:9200] RE: 9171] API 530 Solution annealing after coiling of SA213 TP304H
To: materials-welding@googlegroups.com
Date: Thursday, January 13, 2011, 6:19 AM

Mr. Karthik,
 
What's the design code, API-530 or API-560?
 
I browsed through both the documents(2002/2004 editions),API- 530 is more of a calculation/design guideline while 560 is looks to be a design and fabrication specification.
 
Thanks.
 
Pradip Goswami,P.Eng.
Welding & Metallurgical Specialist & Consultant
Email-pgoswami@sympatico.ca,
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Karthik
Sent: Monday, January 10, 2011 9:22 PM
To: materials-welding@googlegroups.com
Subject: [MW:9171] API 530 Sollution annealing after coiling of SA213 TP304H

Dear All,
Please give your views on below quirey.
Material: SA213 TP304H- Tube-Dia-101.6x8.55mm
Code: API530.
The above material has sollution annealed at 1040 degree celsius from material manufacturer.We are going to make coiling of these tubes(Coil Dia-3.5Mx8M(height) ).
Quirey:
01. Does sollution annealing to be done again after coiling of these tubes? because our customer asked us to do Sollution annealing after coiling.(they referred to ASME Sec.II-Part-A)Also our customer not aware of API530 requirements.Also I dont have API530 book.
 
02.Please give, is there is any requirement as per API530?

Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34916] Applicability of Impact requirement as per ASME B31.3

Dear All, Design code – ASME B31.3, Welding Code- ASME BPVC SEC IX Material  to be used used during Fabrication - SA 333Gr6 (P No.1 G...