Guys

 

OK the correct answer is yes you can based on the grouping process of ASME but we all know ASME is simply a mechanical code and does NOT cover the corrosion resistance aspects ( exception the weld over lay section)

 

Most contractors who specify or use SDSS are utilising the material due to its good corrosion resistance properties and therefore a G48 should be carried out on the Welder Performance – As the SDSS welder performance is required at 48 degrees C the SS qualification will fail.

 

On ALL my projects for the Duplex families you qualify the material to be welded as the ASME in this case is too wide in its use.

 

To continue you also need much tighter control of the Heat Inputs , Gas shield and purge , Cleanliness , Handling , etc etc – It is not correct to group in this instance.

 

A.CLUBB

 

 

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of E.S.Mani
Sent: 17 January 2011 02:12
To: materials-welding@googlegroups.com
Subject: Re: [MW:9252] WQT for Duplex SS

 

Hi Sujay,
As per sec.IX, SS welder is Qualified to weld the SDSS, nut you check with the client spec. also, bcz they will restrict this one.

Regards,

Mani.

On Sun, Jan 16, 2011 at 2:46 PM, PBR <pbrerode@gmail.com> wrote:

Dear Sujay,

          As per to the base metal grouping (ASME SEC IX QW-423.1),F number grouping (QW-432) no changes and so no need of separate qualification, but check other essential variables regarding welder performance refer QW-416.

 

With Regards,

P.Balajirajan.

 

 

-------Original Message-------

 

From: sujay kumar

Date: 1/16/2011 12:59:37 PM

Subject: [MW:9239] WQT for Duplex SS

 

Dear All,

 

 Welder is qualified in SS material,it required separately  to be qualified for Duplex SS material.

 

thanks and regards

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

FREE winter Photo Animations for your email – by IncrediMail

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.




--


Regards,

E.Subramanian

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

***************************************************************************************************************************************************************************
This e-mail (which includes any files attached to it), it is intended solely for the named recipient and may contain CONFIDENTIAL, legally privileged or trade
secret information protected by law. It has been sent it via the internet and is therefore not secure against corruption, interception or unauthorised modification.

If you are not the intended recipient please do not read, use, disclose, distribute, copy, print or rely on any information contained in this e-mail. Please
immediately notify us by telephoning +44 (0) 1494 887808 or return it to us by e-mail to the sender, confirming that this e-mail has been deleted from
your system and any hard copies destroyed.

To the extent permitted by law, neither we nor any of our subsidiaries, parent entities or other affiliates, nor any employee, director or officer thereof,
accepts any liability whatsoever in relation to this e-mail including liability arising from any external breach of security or confidentiality or for virus
infection or for statements made which are clearly the sender's own and not made on our behalf.

"We" and "our" in this footer refer to the following legal entity:

VWS Westgarth Ltd. Registered in Scotland No. 147604, Orbital House, 3 Redwood Crescent, East Kilbride, G74 5PR

This company is a member of the Veolia Water Solutions & Technologies group, but please contact the sender should you have any question
regarding the legal entity on whose behalf this email was sent.
***************************************************************************************************************************************************************************

 ************************************************************************* This e-mail message and any attachments to it are intended only for the  named recipients and may contain confidential information. If you are not one of the intended recipients, please do not duplicate or forward this e-mail message and immediately delete it from your computer. If you  received this email in error, please notify postmaster@veoliawater.com *************************************************************************       

No comments:

[MW:34916] Applicability of Impact requirement as per ASME B31.3

Dear All, Design code – ASME B31.3, Welding Code- ASME BPVC SEC IX Material  to be used used during Fabrication - SA 333Gr6 (P No.1 G...