Generally, hardness shall be checked at the fluid contact surface. However, i suppose the hardness would had been checked on the unexposed surface. Normally, hardness on the root if it is single side weld is lesser than the hardness on the unexposed surface. As the root layer undergoes many heating cycles caused by the deposition of subsequent weld layers. Moreover, the hardness shall be always checked after grinding little bit of top layer/ capping pass.
 
You may run a coupon with similar parameters and perfom a test on the root side (Process side). If it gets passed, then you can convince your client.
 
If the hardness is to be checked on the outer surface which could be yours process exposed side, then grind the final layer, to an extent that it doesn't encrotch below the base metal thickenss, and perform the hardness test again at minimum two locations.

 
Dokku Ajay Kumar
Mobile: +966 500071054



From: Kathalingam Babu <kathalingam.qaqc@ppl.com.sg>
To: materials-welding@googlegroups.com
Sent: Mon, January 17, 2011 3:53:31 AM
Subject: Re: [MW:9248] Hardness Issue

Hi
 
It has to satisfy the requirement of H.7.3.3 (Page 113) of API 5L spec (2010 Ed.),
 
Thanks & Regards,
 
K. Babu
 

----- Original Message -----
Sent: Sunday, January 16, 2011 2:44 PM
Subject: Re: [MW:9235] Hardness Issue

Clava,
 
Just take 2,3 reading just near to high hardness value and check weather it repeats or not.If it does not repeat you can convince ur client.
 
Regards,
 
Manish Kulkanri

--- On Sat, 15/1/11, Eduardo Calva <eduardocalva@hotmail.com> wrote:

From: Eduardo Calva <eduardocalva@hotmail.com>
Subject: [MW:9228] Hardness Issue
To: materials-welding@googlegroups.com
Date: Saturday, 15 January, 2011, 11:40 PM


Dears:
 
Could you please tell me what can I do to solve this issue?:
 
1.- HV hardness requirement for X-60 1" wt pipeline girth welds: 248 HV
2.- Of 15 measurements one value reached 285 HV .
3.- The weld is under water righ now.
 
How can we solve this?, I think just to support, because we can't take the pipe out.
 
Regards.


Eduardo Calva



  > --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34866] Presentation for WPS ,PQR AND WPQ as per ASME Sec IX in power point

Dear Experts.        If anyone having presentation of WPS,PQR and WPQ  as per ASME  SEC.IX  in power point then please share . Regards Sanja...