Re: [MW:9375] Double V

Only thing you can do is wele with single V, then grind the root &
weld the grinded portion. If you see the macro section, it will look
almost double V.

On 1/21/11, Elshan Feyzullayev <elshan_f@hotmail.com> wrote:
>
> it is not practical to do double vee on 4 mm plate. even no V is required
> for this thicknesses as the square butt weld joint confisuration are also
> aceptable.
>
> regards,
> elshan.
>
> Date: Fri, 21 Jan 2011 14:17:57 +0530
> Subject: [MW:9367] Double V
> From: pushprajanand34@gmail.com
> To: materials-welding@googlegroups.com
>
> CAN ANY BODY TELL ME THE PROCEDURE OF MAKEING DOUBLE V ON 4 MM STAINLESS
> STEEL PLATE
> --
> Regards,
> Pushpraj Anand
>
>
>
>
> --
>
> To post to this group, send email to materials-welding@googlegroups.com
>
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
>
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>

--
Sent from my mobile device

Sukamal

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:34913] Filler wire

E71T-1C  is Charpy Impact tested at -20degC E71T-1CJ is Charpy impact tested at -40degC. AWS Classification for FCAW is only a supplementary...