Re: [MW:17383] PRE HEAT PROCEDURE OF E 7016 -1 ELECTRODE

Mr. Lijilal,

a. Please check up the date of manufacturing of the electrode. Generally up to 12 months is OK, but not for
    xay quality welds. 6 months  from manf. date should be better.

b. Dry the electrodes at 300 deg. C  for min. 2 hrs and not the total duration.

c. If required dry them at 350 deg. C for 1 hour and see the results. may be it should be OK.

d. Change the brand if it is also  not working  out.

Sridhar.


From: jiji lal <jijilalkm@gmail.com>
To: materials-welding@googlegroups.com
Sent: Saturday, 13 April 2013 10:36 AM
Subject: [MW:17372] PRE HEAT PROCEDURE OF E 7016 -1 ELECTRODE

SIR,

I'm engaged with welding of API 5LX 80  grade pipeline for regassified LNG transmission . We do  Tie-in method using SMAW+FCAW.
For root pass welding we use E7016-1 electrode after pre heating 250 degree for 2 hr in mother oven and maintain 100 degree in holding oven . during RT interpretation severe hollow bead and porosity observed in root .hence PMC sent almost all joints for repair.now it becomes a serious issue and I think ,the pre heat method was not proper. kindly advice me in this issue.

Mr.Jijilal k .m
qa/qc dept. tecpro ltd.
kochi.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 


No comments:

Re: [MW:34913] Filler wire

E71T-1C  is Charpy Impact tested at -20degC E71T-1CJ is Charpy impact tested at -40degC. AWS Classification for FCAW is only a supplementary...