Dear Hegde Sir

How do we measure the Percentage while mixing up the used and fresh flux,because sometime client may object for mixing of flux.





Mahendra arya




On Fri, Apr 19, 2013 at 10:14 AM, Prakash Hegde <pb.hegde@yahoo.com> wrote:
Dear Maulik
There is no problem of Solid wire which are returned from shop to stores -This can bekept in stores with record after ensuring the correctness of returned  consumables
b) For SAW flux -return flux to be stored separately in a drum with its batch no and the same can be mixed with Fresh Flux in the ratio of 75% to 25% for Baking and Holding This system should be addressed in your Manual
c)For Electrodes-It will be difficult to maintain record for baking and holding due to its variety and number of batches from, Threfore it is better to use these electrodes for Welding Fixtures and Training and qualification which you can address in Manual
 
Regards
 
Hegde P.B.

--- On Wed, 17/4/13, Maulik Thakkar <mlkthakkar2@gmail.com> wrote:

From: Maulik Thakkar <mlkthakkar2@gmail.com>
Subject: [MW:17454] Welding consumable Return System
To: "Materials & Welding" <materials-welding@googlegroups.com>
Date: Wednesday, 17 April, 2013, 8:23 PM


Dear all,
Can any one help me out to give reference standard for storage, handling and redrying/rebaking of covered electrodes.
Specifically interested for consumable return, rebaking and reissue system (color coding).
Thanks and Regards,
Maulik Thakkar
Welding Engineer
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

No comments:

[MW:34866] Presentation for WPS ,PQR AND WPQ as per ASME Sec IX in power point

Dear Experts.        If anyone having presentation of WPS,PQR and WPQ  as per ASME  SEC.IX  in power point then please share . Regards Sanja...